研究文章
钢纤维的力学性能和Nanosilica面包屑橡胶改性混凝土
表4
结果标本的抗压和抗拉强度测试分割在28 d(单位:MPa)。
|
| 集团 |
C-28 d |
CAvg-28 |
T-28 d |
TAvg-28 |
|
| C35CR5 |
|
|
|
|
|
|
|
|
| 1 sf0 |
40.0 |
37.7 |
38.3 |
38.7 |
2.8 |
2.9 |
3.0 |
2.9 |
| 1 sf0.5 |
44.0 |
42.9 |
41.6 |
42.8 |
3.3 |
3.6 |
3.1 |
3.3 |
| 1 sf1 |
46.8 |
44.5 |
42.4 |
44.6 |
4.9 |
4.7 |
5.2 |
4.9 |
| 1 sf1.5 |
38.9 |
38.8 |
42.3 |
40.0 |
4.6 |
4.0 |
4.6 |
4.4 |
| 1 sf1ns1 |
47.1 |
47.9 |
46.3 |
47.1 |
5.3 |
4.8 |
5.2 |
5.1 |
| 1 sf1ns2 |
49.0 |
46.6 |
46.4 |
47.3 |
5.2 |
4.9 |
5.5 |
5.2 |
|
| C45CR5 |
|
|
|
|
|
|
|
|
| 2 sf0 |
50.1 |
51.1 |
50.8 |
51.3 |
3.4 |
3.3 |
3.4 |
3.3 |
| 2 sf0.5 |
54.7 |
51.9 |
51.8 |
52.8 |
3.7 |
3.4 |
3.8 |
3.6 |
| 2 sf1 |
53.3 |
54.8 |
52.5 |
53.5 |
4.2 |
4.9 |
4.3 |
4.4 |
| 2 sf1.5 |
57.6 |
54.6 |
50.7 |
54.3 |
4.8 |
4.9 |
5.4 |
5.0 |
| 2 sf1ns1 |
54.1 |
55.1 |
55.0 |
54.9 |
4.8 |
5.3 |
5.3 |
5.1 |
| 2 sf1ns2 |
56.1 |
58.4 |
53.7 |
56.1 |
4.9 |
5.2 |
4.6 |
4.9 |
|
| C45CR10 |
|
|
|
|
|
|
|
|
| 3 sf0 |
50.0 |
49.8 |
52.7 |
50.8 |
3.6 |
2.9 |
3.0 |
3.2 |
| 3 sf0.5 |
53.6 |
49.2 |
50.9 |
51.2 |
4.3 |
4.2 |
3.3 |
3.9 |
| 3 sf1 |
55.0 |
53.5 |
51.7 |
53.4 |
4.5 |
3.6 |
4.0 |
4.0 |
| 3 sf1.5 |
50.0 |
48.8 |
51.1 |
50.0 |
4.0 |
4.9 |
3.7 |
4.0 |
| 3 sf1ns1 |
52.7 |
51.5 |
49.7 |
51.3 |
3.9 |
3.8 |
3.9 |
3.9 |
| 3 sf1ns2 |
51.5 |
52.1 |
53.6 |
52.4 |
3.7 |
3.9 |
3.5 |
3.7 |
|
|